Coatings

HY Series Organic Bentonite Use Method

HY series organic bentonite is made by excellent bentonite with the processing of highly purified, modified and ion exchange into organic covering agent, it is a sheet structure product, if you want the organic bentonite to play a better performance, you need to separate its sheet-structure as much as possible. This process usually needs to be provided with mechanical energy, chemical energy and heat energy.

Use Method:

Dry powder method:

Dry powder method is that add the dry powder directly into the system during the production process, it doesn't need the polar activator, such as HY-2, HY-S2, HY-S3, HY-S34.

Pre gel method:

For poor wettability resin systems (such as epoxy, polyester, short oil alkyd resin etc. )it is better to use HY series organic bentonite by pre gel. 

(1) composed of pre gel: solvent 87%, organic bentonite 8-10%, polar activator 3-4%.

(2) preparation of pre gel: solvent and organic bentonite (mixed 10min, fully wettability), then add the polar activator (stirring for 5min, full expansion). 

Other information:

The dispersion speed

No matter you use any one method, bentonite products must be thoroughly dispersed to be a gel, so it can show its properties as thixotropy, anti settling and thickening effect, this kind of dispersion need extra high shear force, for example, to use high speed dispersion machine, three roller mill, colloid mill, sand grinding or milling. If the shear force and activation energy is enough, it is easy to obtain gel. The organic bentonite efficiency increased with the increase of dispersion speed.

Dispersion temperature

Increasing the temperature can also improve the gel property. The gel property with high temperature solvent is better than the low temperature (0 °C -5 °C ) solvent when the other conditions keep the same. But the dispersion temperature can not exceed the boiling point of activation solvent.

Activating agent

The polar additive can help the sheet-layer structure bentonite easily form a layer-sheet structure, thus formed a thixotropic gel, polar additives such as ethanol, methanol, acetone, propylene carbonate, the add amount of polar additives is generally 30%-50% of the organic bentonite.

Moisture

Organic bentonite must have enough moisture to develop into a network structure pre gel, the water molecules forming a bridge for the network structure, so the organic bentonite should not be too dry, the general moisture content should be around 3.5%, polar additives should not use anhydrous, the suitable content of the polar additives is appropriate 95% (the moisture is 5%).


主站蜘蛛池模板: 窝窝午夜看片| 熟妇熟女乱妇乱女网站| 亚洲aⅴ天堂av天堂无码app| 正在播放的国产a一片| 嗯~啊~轻一点??视频| 日日噜噜夜夜狠狠久久蜜桃| 东京热久久综合伊人av| 久久国产成人午夜av影院| 亚洲日韩v无码中文字幕| av天堂久久精品影音先锋 | 在国产线视频a在线视频| 男女性杂交内射女bbwxz| 国产精品厕所| 精品无人乱码高清在线观看| 欧美白胖bbbbxxxx| 无码精品久久久天天影视| 久久99精品国产99久久6尤物| 亚洲一区在线日韩在线秋葵| 在线亚洲日产一区二区| 女人被男人爽到呻吟的视频| 免费无码又爽又刺激成人| 激情综合婷婷丁香五月| 国内精品久久毛片一区二区| 国产一卡2卡3卡四卡精品国色无边 | 亚洲综合另类小说色区大陆| 在线最全导航精品福利av| 国产成人欧美亚洲日韩电影| 久久久久久亚洲精品不卡| 无码人妻丰满熟妇精品区| 久久国产午夜精品理论片| 亚洲aⅴ无码成人网站国产app| 亚洲欧美人成网站aaa| 亚洲gv猛男gv无码男同短文| 亚洲欧洲日产国码无码av喷潮| 2018高清国产一区二区三区| 亚洲成成品网站源码中国有限公司 | 久久大香香蕉国产免费网动漫 | 欧美丰满大爆乳波霸奶水多| 久久久亚洲一区二区三区| 亚洲性视频免费视频网站| 国产精品久久国产精品99 gif|